MATERIAL FINER THAN 75μ OF FINE AGGREGATE

 AIM:-

  • Determination Of Material Finer Than 75μ Of fine Aggregate
  • As Per IS:2386 (Part- 1)

APPARATUS:-


  • WT Balance
  • IS sieve -75μ
  • Upper 1.18 mm (sieve-IS-460)
  • Container pan type
  • Hot Air Oven (temp. 110⁰C ± 5)
  • SAMPLE IS:2430

PROCEDURE:-

  • The test sample shall be dried to content weight at a temperature of 110°c ± 5 and weight the nearest 0.1 percent.
  • The test sample after being dried and weight shall be placed in the container and sufficient water added to cover it. the contents of the container shall be agitated vigorously.
  • The agitation shall be sufficiently vigorous to result in the complete separation from the coarse particle of all particle finer than 75 u and bring the fine material into suspension.
  • Care shall be taken to avoid as much as possible,the decantation of the coarse particle of the sample, the operation shall be repeated until the wash water is clear.
  • The wash water containing the suspended and dissolved solids shall be immediately poured over the nested sieves arranged with the coarse sieve on the top.
  • All the material retained on the nested sieve shall be returned to the washed sample the washed aggregate shall be dried to the constant weight at a temperature not exceeding 110 °c and weight to the nearest 0.1 percent.
CALCULATIONS:- 
  • The amount of material passing the is sieve Shall be calculated as- 

LIMIT:- 
  • Natural Sand not more than 3% & Crusher Sand not more than 15% & Manufacturing Sand not more than 10%.